Friday, November 23, 2012

Silicone


Application:

Electric parts
Lubricants

SI Glass fiber

Molding properties

Drying temperature                                          : —
Drying time                                                      : —
Injection forming cylinder temperature              : —
Injection molding tool temperature                    : —
Injection molding pressure                                : —
Compression molding temperature                    : 154~182°C
Compression molding pressure                         : 70.3~350kgf/cm2
Molding shrinkage rate                                     : 0~0.5%
Specific gravity                                                 : 1.80~1.94density
                JIS            : K6911,K7122
                A.S.T.M   : D792

Mechanical characteristics

Tensile strength                                               : 281~457kgf/cm2
               JIS            : K6911,K7113
              A.S.T.M   : D638
Tensile elongation                                           : —
Compressive strength                                     : 103~1050kgf/cm2
               JIS            : K7208
Flexure strength                                              : 703~984kgf/cm2
              JIS            : K7203
Izot impact strength                                        : 1.63~43.5kgf/cm2
             JIS            : K7110,K7111
Rockwell hardness                                          : M80~90
            JIS            : K7202
            A.S.T.M   : D785

Thermal characteristic

Heat resistance temperature (continuous)   : >315°C
Deflection temperature under load
         a) Bending stress18.6kgf/cm2               : >482°C
         b) Bending stress 4.6kgf/cm2                : —
                 JIS            : K7206,K7207
                 A.S.T.M   : D648

Urea-formaldehyde


Application:

Laminated sheets
Textile
Colorant
Knobs
Tableware


Molding properties

Drying temperature                                           : —
Drying time                                                       : —
Injection forming cylinder temperature                : 143~160°C
Injection molding tool temperature                     : —
Injection molding pressure                                 : 1050~1410kgf/cm¬¬2
Compression molding temperature                     : 135~176°C
Compression molding pressure                          : 141~562kgf/cm2
Molding shrinkage rate                                      : 0.6~1.4%
Specific gravity                                                 : 1.47~1.52density
        JIS            : K6911,K7122
        A.S.T.M   : D792

Mechanical characteristics

Tensile strength                                              : 387~914kgf/cm2
                JIS            : K6911,K7113
                A.S.T.M   : D638
Tensile elongation                                           : 0.5~1.0%
Compressive strength                                     : 176~316kgf/cm2
               JIS            : K7208
Flexure strength                                              : 703~1270kgf/cm2
              JIS            : K7203
Izot impact strength                                        : 1.36~2.18kgf/cm2
              JIS            : K7110,K7111
Rockwell hardness                                          : M10~120
              JIS            : K7202
              A.S.T.M   : D785

Thermal characteristic

Heat resistance temperature (continuous)          : 76.5°C
Deflection temperature under load
        a) Bending stress18.6kgf/cm2                       : 126~143°C
        b) Bending stress 4.6kgf/cm2                        : —
               JIS            : K7206,K7207
               A.S.T.M   : D648

Saturday, October 29, 2011

POM-GF glass fiber 25% or less


Application:
          · Motor fans
          · Pump 
          · Gears
          · Switch covers


Molding Properties
          · Drying temperature                                     : 110°C
          · Drying time                                                 : 2hr
          · Injection forming cylinder temperature         : 180~230°C
          · Injection molding tool temperature               : 60~120°C
          · Injection molding pressure                           : 730~1410kgf/cm­­2
          · Compression molding temperature               : —
          · Compression molding pressure                    : —
          · Molding shrinkage rate                                : 0.4%
          . Specific gravity                                            : 1.61density
          JIS            : K6911,K7122
          A.S.T.M        : D792


Mechanical Characteristics
          · Tensile strength                                           : 1250~1300kgf/cm2
          JIS            : K6911,K7113
          A.S.T.M        : D638
          · Tensile elongation                                       : 3%
          · Compressive strength                                 : 1200kgf/cm2
         JIS            : K7208
          · Flexure strength                                          : 1970kgf/cm2
         JIS            : K7203
          · Izot impact strength                                     : 10kgf/cm2
         JIS            : K7110,K7111




POM General




Application:
            ·         Gears
            ·         Bearing
            ·         Electromagnetic valve cases
            ·         Connector

Molding Properties
            ·         Drying temperature                                           : 10°C
            ·         Drying time                                                       : 2hr
            ·         Injection forming cylinder temperature               : 180~230°C
            ·         Injection molding tool temperature                     : 60~120°C
            ·         Injection molding pressure                                 : 703~1410kgf/cm­­2
            ·         Compression molding temperature                     : —
            ·         Compression molding pressure                          : —
            ·         Molding shrinkage rate                                      : 2~2.5%
            ·         Specific gravity                                                  : 1.41~1.42density
            JIS            : K6911,K7122
            A.S.T.M   : D792

Mechanical Characteristics
            ·         Tensile strength                                               : 580~800kgf/cm2
             JIS            : K6911,K7113
             A.S.T.M   : D638
            ·         Tensile elongation                                           : 25~75%
            ·         Compressive strength                                     : 1270kgf/cm2
             JIS            : K7208
            ·         Flexure strength                                              : 991kgf/cm2
             JIS            : K7203
            ·         Izot impact strength                                        : 5.4~13kgf/cm2
             JIS            : K7110,K7111
            ·         Rockwell hardness                                          : M78~94
             JIS            : K7202
             A.S.T.M   : D785

Thermal Characteristic
             ·         Heat resistance temperature (continuous)         : 90°C
             ·         Deflection temperature under load              
    a)      Bending stress               18.6kgf/cm2                         : 124°C
    b)      Bending stress               4.6kgf/cm2                           : 170°C
             JIS            : K7206,K7207
             A.S.T.M   : D648




Sunday, August 14, 2011

Unsaturated polyester Glass fiber SMC



Molding Properties
          ·         Drying temperature                               : —
          ·         Drying time                                           : —
          ·         Injection forming cylinder temperature   : —
          ·         Injection molding tool temperature         : —
          ·         Injection molding pressure                     : —
          ·         Compression molding temperature         : 132~176°C
          ·         Compression molding pressure              : 21.1~94.4kgf/cm2
          ·         Molding shrinkage rate                          : 0.1~0.4%
          ·         Specific gravity                                      : 1.65~2.60density
               JIS            : K6911,K7122
               A.S.T.M   : D792


Mechanical Characteristics
           ·         Tensile strength                                        : 562~1410kgf/cm2
             JIS            : K6911,K7113
             A.S.T.M   : D638
           ·         Tensile elongation                                    : 3%
           ·         Compressive strength                              : 1050~2110kgf/cm2
             JIS            : K7208
           ·         Flexure strength                                      : 703~2530kgf/cm2
            JIS            : K7203
           ·         Izot impact strength                                 : 38.1~120kgf/cm2
            JIS            : K7110,K7111
           ·         Rockwell hardness                                  : barcol 50~70
            JIS            : K7202
            A.S.T.M   : D785


Thermal Characteristic
            ·         Heat resistance temperature (continuous)   : 149~204°C
            ·         Deflection temperature under load
                      a)      Bending stress18.6kgf/cm2               : 190~260°C
                      b)      Bending stress 4.6kgf/cm2                : —
              JIS            : K7206,K7207
              A.S.T.M   : D648

Unsaturated Polyester Glass fiber Premix


Molding Properties
            ·         Drying temperature                                     : —
            ·         Drying time                                                 : —
            ·         Injection forming cylinder temperature         : —
            ·         Injection molding tool temperature               : —
            ·         Injection molding pressure                           : —
            ·         Compression molding temperature               : 138~176°C
            ·         Compression molding pressure                    : 35.2~141kgf/cm2
            ·         Molding shrinkage rate                                : 0.1~1.2%
            ·         Specific gravity                                            : 1.65~2.30density
                 JIS            : K6911,K7122
                A.S.T.M   : D792


Mechanical Characteristics
            ·         Tensile strength                                      : 211~703kgf/cm2
               JIS            : K6911,K7113
               A.S.T.M   : D638
            ·         Tensile elongation                                   : 0.5~2.0%
            ·         Compressive strength                             : 1410~2110kgf/cm2
               JIS            : K7208
            ·         Flexure strength                                      : 492~1410kgf/cm2
               JIS            : K7203
            ·         Izot impact strength                                 : 8.16~87.1kgf/cm2
               JIS            : K7110,K7111
            ·         Rockwell hardness                                  : barcol 50~80
               JIS            : K7202
               A.S.T.M   : D785


Thermal Characteristic
             ·         Heat resistance temperature (continuous)   : 149~176°C
             ·         Deflection temperature under load
                       a)      Bending stress18.6kgf/cm2               : >204°C
                       b)      Bending stress 4.6kgf/cm2                : —
                JIS            : K7206,K7207
                A.S.T.M   : D648





Unsaturated Polyester

Applications:

          ·         TV tuners
          ·         Fuses
          ·         Breakers
          ·         Motor covers
          ·         Power distributor case covers
          ·         Press rings
          ·         Rectifier frames

Unsaturated Polyester Glass roving

Molding Properties

          ·         Drying temperature                                        : —
          ·         Drying time                                                    : —
          ·         Injection forming cylinder temperature            : —
          ·         Injection molding tool temperature                  : —
          ·         Injection molding pressure                              : —
          ·         Compression molding temperature                  : 76.5~160°C
          ·         Compression molding pressure                       : 17.6~141kgf/cm2
          ·         Molding shrinkage rate                                   : 0.02~0.2%
          ·         Specific gravity                                               : 1.35~2.30density
              JIS            : K6911,K7122
              A.S.T.M   : D792

Mechanical Characteristics

          ·         Tensile strength                                        : 1050~2110kgf/cm2
             JIS            : K6911,K7113
             A.S.T.M   : D638
          ·         Tensile elongation                                    : 0.5~5.0%
          ·         Compressive strength                              : 1050~2110kgf/cm2
             JIS            : K7208
          ·         Flexure strength                                       : 703~1270kgf/cm2
             JIS            : K7203
          ·         Izot impact strength                                 : 10.9~109kgf/cm2
             JIS            : K7110,K7111
          ·         Rockwell hardness                                  : barcol 50~80
             JIS            : K7202
             A.S.T.M   : D785

Thermal Characteristic

           ·         Heat resistance temperature (continuous)       : 149~176°C
           ·         Deflection temperature under load
                     a)      Bending stress18.6kgf/cm2                   : >204°C
                     b)      Bending stress 4.6kgf/cm2                    : —
             JIS            : K7206,K7207
             A.S.T.M   : D648